				name
			 | 
			
				brand
			 | 
			
				Alloy elements %
			 | 
			
				use
			 | 
			
				Add the amount
			 | 
			
				Using temperature ℃
			 | 
			
				performance
			 | 
		
		
			| 
				Aluminum bronze
			 | 
			
				 
					ALCu50 
				 
			 | 
			
				Cu48~52
			 | 
			
				Adjust alloy composition
			 | 
			
				Needs vary
			 | 
			
				570~600
			 | 
			
				crispy
			 | 
		
		
			| 
				al-si
			 | 
			
				ALSi20
			 | 
			
				Si18~20
			 | 
			
				Adjust alloy composition 
			 | 
			
				Needs vary 
			 | 
			
				700~800
			 | 
			
				crispy 
			 | 
		
		
			| 
				Aluminum manganese
			 | 
			
				ALMn10
			 | 
			
				Mn9~11
			 | 
			
				Adjust alloy composition 
			 | 
			
				Needs vary 
			 | 
			
				770~830
			 | 
			
				toughening
			 | 
		
		
			| 
				Aluminum manganese
			 | 
			
				ALMn20
			 | 
			
				Mn18~22
			 | 
			
				Adjust alloy composition 
			 | 
			
				Needs vary 
			 | 
			
				780~850
			 | 
			
				toughening 
			 | 
		
		
			| 
				Aluminum  titanium
			 | 
			
				ALTi5
			 | 
			
				Ti4~6
			 | 
			
				Grain refinement to improve plasticity 
			 | 
			
				Needs vary 
			 | 
			
				1020~1070
			 | 
			
				Easy segregation
			 | 
		
		
			| 
				Aluminum  titanium 
			 | 
			
				ALTi10
			 | 
			
				Ti9~11
			 | 
			
				Grain refinement to improve plasticity
			 | 
			
				Needs vary 
			 | 
			
				1020~1070
			 | 
			
				Easy segregation 
			 | 
		
		
			| 
				Aluminum and nickel
			 | 
			
				ALTi10 
			 | 
			
				Ni9~11
			 | 
			
				To improve the plastic
			 | 
			
				Needs vary 
			 | 
			
				680~730
			 | 
			
				toughening
			 | 
		
		
			| 
				Aluminium chromium
			 | 
			
				ALCr5
			 | 
			
				Cr4~6
			 | 
			
				Improve plasticity and performance
			 | 
			
				Needs vary 
			 | 
			
				900~1000
			 | 
			
				Easy segregation 
			 | 
		
		
			| 
				Aluminium chromium
			 | 
			
				ALCr10
			 | 
			
				Cr9~11
			 | 
			
				Improve plasticity and performance 
			 | 
			
				Needs vary 
			 | 
			
				900~1000
			 | 
			
				Easy segregation 
			 | 
		
		
			| 
				Aluminium chromium
			 | 
			
				ALCr20
			 | 
			
				Cr18~22
			 | 
			
				Improve plasticity and performance 
			 | 
			
				Needs vary 
			 | 
			
				910~1020
			 | 
			
				Easy segregation 
			 | 
		
		
			| 
				Aluminium zirconium
			 | 
			
				ALZr5
			 | 
			
				Zr4~6
			 | 
			
				Improve plasticity and performance 
			 | 
			
				Needs vary 
			 | 
			
				800~850
			 | 
			
				Easy segregation 
			 | 
		
		
			| 
				Aluminum  antimony
			 | 
			
				ALSb4
			 | 
			
				Sb3~5
			 | 
			
				Improve plasticity and performance 
			 | 
			
				Needs vary 
			 | 
			
				660
			 | 
			
				Easy segregation 
			 | 
		
		
			| 
				Aluminum  antimony 
			 | 
			
				ALSb10
			 | 
			
				Sb9~11
			 | 
			
				Improve plasticity and performance 
			 | 
			
				Needs vary 
			 | 
			
				660
			 | 
			
				Easy segregation 
			 | 
		
		
			| 
				Aluminum and iron
			 | 
			
				ALFe20
			 | 
			
				Fe18~22
			 | 
			
				Improve plasticity and performance 
			 | 
			
				Needs vary 
			 | 
			
				1020
			 | 
			
				crispy
			 | 
		
		
			| 
				Aluminum and beryllium
			 | 
			
				ALBe1
			 | 
			
				Be0.9~1.2
			 | 
			
				Improve plasticity and performance 
			 | 
			
				Needs vary 
			 | 
			
				820
			 | 
			
				crispy
			 | 
		
		
			
				Aluminum and beryllium 
			 | 
			
				ALBe3
			 | 
			
				Be2~4
			 | 
			
				Improve plasticity and performance 
			 | 
			
				Needs vary 
			 | 
			
				820
			 | 
			
				crispy
			 | 
		
		
			
				Aluminum and beryllium 
			 | 
			
				ALBe5
			 | 
			
				Be4.5~5.5
			 | 
			
				Improve plasticity and performance 
			 | 
			
				Needs vary 
			 | 
			
				820
			 | 
			
				crispy
			 | 
		
		
			| 
				Aluminum boron
			 | 
			
				ALB3
			 | 
			
				B2.5~3.5
			 | 
			
				Reduce the resistivity, improve the conductivity, grain refinement
			 | 
			
				2~4%
			 | 
			
				800
			 | 
			
				crispy
			 | 
		
		
			| 
				Aluminum titanium boron (piece/wire)
			 | 
			
				ALTi5B1
			 | 
			
				 
					Ti4.5~6   B0.9~1.2 
				 
			 | 
			
				Grain refinement
			 | 
			
				0.5~2‰
			 | 
			
				800
			 | 
			
				Easy segregation 
			 | 
		
		
			| 
				Rare earth aluminum
			 | 
			
				ALRe10
			 | 
			
				Re9~11
			 | 
			
				Grain refinement 
			 | 
			
				2~3‰ 
			 | 
			
				680
			 | 
			
				Easy segregation 
			 | 
		
		
			| 
				Alti boron rare earth
			 | 
			
				ALTi5B1Re10
			 | 
			
				Ti5B1Re10
			 | 
			
				Grain refinement 
			 | 
			
				1~3‰ 
			 | 
			
				800
			 | 
			
				Easy segregation 
			 | 
		
		
			| 
				Titanium aluminum carbon
			 | 
			
				ALTi5C0.2
			 | 
			
				Ti5C0.2
			 | 
			
				Grain refinement 
			 | 
			
				1~2‰ 
			 | 
			
				1020~1070
			 | 
			
				Easy segregation 
			 | 
		
		
			| 
				Aluminum strontium
			 | 
			
				ALSr10
			 | 
			
				Sr9~11
			 | 
			
				For long - term modification of aluminum - silicon alloys under 13% silicon
			 | 
			
				1~2‰ 
			 | 
			
				680~740
			 | 
			
				Easy segregation 
			 | 
		
		
			| 
				Yttrium aluminum
			 | 
			
				ALY5
			 | 
			
				Y4~6
			 | 
			
				Improve plasticity and performance
			 | 
			
				1~2‰ 
			 | 
			
				740~800
			 | 
			
				Easy segregation 
			 | 
		
		
			| 
				Aluminum bismuth
			 | 
			
				ALBi10
			 | 
			
				Bi9~11
			 | 
			
				Improve plasticity and increase fluidity
			 | 
			
				1~2‰ 
			 | 
			
				700~710
			 | 
			
				Easy segregation 
			 | 
		
		
			| 
				Aluminum scandium
			 | 
			
				ALSc2
			 | 
			
				Sc
			 | 
			
				Adjust the alloy composition and improve the alloy performance
			 | 
			
				Needs vary 
			 | 
			
				700-800
			 | 
			
				toughening 
			 | 
		
		
			| 
				Aluminum cobalt
			 | 
			
				ALCo5
			 | 
			
				Co
			 | 
			
				Adjust the alloy composition and improve the alloy performance
			 | 
			
				Needs vary 
			 | 
			
				720-750
			 | 
			
				toughening 
			 | 
		
		
			| 
				Aluminum molybdenum
			 | 
			
				ALMo5-10
			 | 
			
				Mo
			 | 
			
				Adjust the alloy composition and improve the alloy performance
			 | 
			
				Needs vary 
			 | 
			
				720-750
			 | 
			
				toughening 
			 | 
		
		
			| 
				Aluminum niobium
			 | 
			
				ALNb10
			 | 
			
				Nb
			 | 
			
				Increase fluidity and improve alloy performance
			 | 
			
				Needs vary 
			 | 
			
				690-750
			 | 
			
				toughening 
			 | 
		
		
			| 
				Aluminum neodymium
			 | 
			
				ALNd30
			 | 
			
				Nd
			 | 
			
				Adjust the alloy composition and improve the alloy performance
			 | 
			
				Needs vary 
			 | 
			
				690-750
			 | 
			
				Easy segregation 
			 | 
		
		
			| 
				Aluminum cerium
			 | 
			
				ALCe10
			 | 
			
				Ce
			 | 
			
				Adjust the alloy composition and improve the alloy performance
			 | 
			
				Needs vary 
			 | 
			
				690-750
			 | 
			
				Easy segregation 
			 | 
		
		
			| 
				Aluminum cadmium
			 | 
			
				ALCd5 / 10
			 | 
			
				Cd
			 | 
			
				Adjust the alloy composition and improve the alloy performance
			 | 
			
				Needs vary 
			 | 
			
				690-750
			 | 
			
				toughening 
			 | 
		
		
			| 
				Aluminum tellurium
			 | 
			
				ALTe5
			 | 
			
				Te
			 | 
			
				Adjust the alloy composition and improve the alloy performance
			 | 
			
				Needs vary 
			 | 
			
				710-740
			 | 
			
				crispy 
			 | 
		
		
			
				The chemical composition and impurities of aluminum intermediate alloy ingots shall be manufactured according to the YS/ t282-2000 standard. 
			 |